19
2024
-
03
Main factors affecting SKF bearing grinding deterioration layer
There are two main factors affecting the grinding metamorphic layer of SKF bearing, which are the grinding force and grinding heat of SKF bearing.
There are two main factors affecting the grinding metamorphic layer of SKF bearing, which are the grinding force and grinding heat of SKF bearing.
1. Grinding force
During grinding, the surface layer of the workpiece will be subjected to the cutting force, compression force and friction force of the grinding wheel. Especially the role of the latter two, so that the workpiece surface layer formed a strong directional plastic deformation layer and work hardening layer. These metamorphic layers must affect the variation of residual stress in the surface layer.
(1) Cold plastic deformation layer
In the grinding process, each moment of abrasive particle is equivalent to a cutting edge. However, in many cases, the front Angle of the cutting edge is negative, and the abrasive particle in addition to the cutting effect is to make the workpiece surface withstand the extrusion action (ploughing action), leaving an obvious plastic deformation layer on the workpiece surface. The degree of deformation of this deformation layer will increase with the degree of grinding bluntness and the increase of grinding feed.
(2) thermoplastic deformation (or high temperature deformation) layer
The instantaneous temperature formed by grinding heat on the working surface makes the elastic limit of the workpiece surface layer at a certain depth drop sharply, and even reach the degree of elasticity disappearance. At this time, the working surface layer is free to stretch under the action of grinding force, especially compression force and friction force, which is limited by the base metal, and the surface is compressed (more), causing plastic deformation in the surface layer. The high temperature plastic deformation increases with the increase of workpiece surface temperature when the grinding process is unchanged.
(3) Work hardening layer
Sometimes using microhardness and metallography can be found, due to processing deformation caused by the surface layer hardness increase.
2, grinding heat
In the grinding process, the contact zone between the grinding wheel and the workpiece consumes a lot of energy and generates a lot of grinding heat, resulting in local instantaneous high temperature in the grinding zone. It can be found that the instantaneous temperature in the grinding zone can reach 1000 ~ 1500℃ within 0.1 ~ 0.001ms by deducing and calculating the theoretical formula of heat transfer of linear moving heat source or measuring the experimental conditions by infrared method and thermocouple method. Such an instantaneous high temperature is enough to make the surface layer at a certain depth of the working surface produce high-temperature oxidation, amorphous microstructure, high-temperature tempering, secondary quenching, and even burn cracking and other changes.
(1) SKF bearing surface oxide layer
Under the action of instantaneous high temperature, the steel surface reacts with oxygen in the air to form an extremely thin (20 ~ 30nm) thin layer of iron oxide. It is worth noting that there is a corresponding relationship between the thickness of oxide layer and the total thickness of surface grinding metamorphic layer. This shows that the oxide layer thickness is directly related to the grinding process and is an important sign of grinding quality.
(2) Amorphous microstructure layer
When the surface of the workpiece reaches a molten state due to the instantaneous high temperature in the grinding zone, the molten metal molecular flow is evenly coated on the working surface and cooled by the base metal at a very fast speed to form an extremely thin layer of amorphous microstructure. It has high hardness and toughness, but it is only about 10nm and is easy to be removed in precision grinding.
(3) high-temperature tempering layer
The instantaneous high temperature in the grinding zone can cause the surface to be heated to a higher temperature than the workpiece tempering heating within a certain depth (10 ~ 100nm). In the case of not reaching the austenitizing temperature, as the heating temperature increases, the surface layer by layer will produce a re-tempering or high-temperature tempering organizational transformation corresponding to the heating temperature, and the hardness will also decrease. The higher the heating temperature, the greater the decrease in hardness.
(4) SKF bearing two-layer quenching layer
When the instantaneous high temperature in the grinding zone heats the workpiece surface layer above the austenitizing temperature (Ac1), the austenitizing structure of the layer is re-quenched into martensitic structure during the subsequent cooling process. Any workpiece with secondary quenching burn, the secondary quenching layer must be a high temperature tempering layer with very low hardness.
(5) Grinding cracks
Secondary quenching burn will change the surface layer stress of the workpiece. The secondary quenching zone is in a state of pressure, and the material in the high-temperature annealing zone below it has a large tensile stress, which is where the crack core is likely to occur. Cracks tend to propagate along the original austenitic grain boundaries. Severe burns can lead to cracks (mostly cracks) on the entire grinding surface, resulting in workpiece abandonment.